Fatigue strength: PH1 steel (Vxx/MSn)

This page presents the S-N curves and fatigue limit of PH1 steel samples that underwent machining that removed allowance of 0.5mm and shot-peening (in that order), obtained using the bending tests of rotating bars with AM layers normal to the axis of rotation.

Production and prost-processing conditions

Build orientation of longitudinal axis vertical
Position with respect to inert gas flow undefined
Post-processing machining allowance 0.5mm → shot-peening

Experimental S-N curve

Experimental method ISO1143, rotating bending test R=-1
AM layers normal to axis of rotation

Wöhler curve

Fatigue limit (MPa) 457
Number of cycles to failure N N=1,02⋅1023⋅S-6,54
Stress amplitude S (MPa) S=3312⋅N-0,153

Explanation of the terms are given at the page Fatigue strength description.