Fatigue strength: MS1 steel (Vxx/Snn)
This page presents the S-N curves and fatigue limit of MS1 steel samples that underwent shot-peening only, obtained using the bending tests of rotating bars with AM layers normal to the axis of rotation.
Production and prost-processing conditions
Build orientation of longitudinal axis | vertical |
---|---|
Position with respect to inert gas flow | undefined |
Post-processing | shot-peening |
Experimental S-N curve
Wöhler curve
Fatigue limit (MPa) | 430 |
---|---|
Number of cycles to failure N | N=1,12⋅10<html>39</html>⋅S<html>-12,20</html> |
Stress amplitude S (MPa) | S=1592⋅N<html>-0,082</html> |