2.dr:2.3.1.2.1.3.1.dmls_sn:hg.cx.vxx.msn
Table of Contents
Fatigue strength: CX steel (Vxx/MSn)
This page presents the S-N curves and fatigue limit of CX steel samples that underwent machining that removed allowance of 0.5mm and shot-peening (in that order), obtained using the bending tests of rotating bars with AM layers normal to the axis of rotation.
Production and prost-processing conditions
Build orientation of longitudinal axis | vertical |
---|---|
Position with respect to inert gas flow | undefined |
Post-processing | machining allowance 0.5mm → shot-peening |
Experimental S-N curve
Wöhler curve
Fatigue limit (MPa) | 446 |
---|---|
Number of cycles to failure N | N=4,29⋅10<html>52</html>⋅S<html>-17,24</html> |
Stress amplitude S (MPa) | S=1129⋅N<html>-0,058</html> |
Explanation of the terms are given at the page Fatigue strength description.
This page is a part of the section DMLS/SLM: Fatigue design rules.
2.dr/2.3.1.2.1.3.1.dmls_sn/hg.cx.vxx.msn.txt · Last modified: 2022/01/10 09:26 by soskicz