This page presents the S-N curves and fatigue limit of MS1 steel samples that underwent shot-peening, heat treatment and machining that removed allowance of 3mm (in that order), obtained using the bending tests of rotating bars with AM layers parallel to the axis of rotation.
| Build orientation of longitudinal axis | horizontal |
|---|---|
| Position with respect to inert gas flow | undefined |
| Post-processing | shot-peening → heat treatment → machining allowance 3mm |
| Fatigue limit (MPa) | 576 |
|---|---|
| Number of cycles to failure N | N=6,35⋅10<html>29</html>⋅S<html>-8,26</html> |
| Stress amplitude S (MPa) | S=4038⋅N<html>-0,121</html> |
Explanation of the terms are given at the page Fatigue strength description.
This page is a part of the section DMLS/SLM: Fatigue design rules.